| Availability: | |
|---|---|
| Quantity: | |
NiCr
MICC
| Main property of NiCr electric heating alloy | ||||||||
| property | type | Cr20Ni80 | Cr30Ni70 | Cr15Ni60 | Cr20Ni35 | Cr20Ni30 | ||
| Main chemical composition% | Ni | Rest | Rest | 55~61 | 34~37 | 30~34 | ||
| Cr | 20~23 | 28~31 | 15~18 | 18~21 | 18~21 | |||
| Fe | Rest | Rest | Rest | |||||
| Max continuous Temp.of element(℃) | 1200 | 1200 | 1150 | 1100 | 1100 | |||
| resistivity(mm²/m) | 1.09 | 1.09 | 1.12 | 1 | 1.04 | |||
| Density((g/cm³)) | 8.4 | 8.4 | 8.2 | 7.9 | 7.9 | |||
| Thermal conductivity(KJ/M.h℃) | 60.3 | 60.3 | 45.2 | 43.8 | 43.8 | |||
| Coefficient of liner expansion(a*10-5/℃) | 18 | 18 | 17 | 19 | 19 | |||
| Melting point (℃) | 1400 | 1400 | 1390 | 1390 | 1390 | |||
| Elongation(%) | 720 | 720 | 720 | 720 | 720 | |||
| Micrographic structure | Austenitic | Austenitic | Austenitic | Austenitic | Austenitic | |||
| Magnetic property | NONE | NONE | NONE | NONE | NONE | |||
| Main property of NiCr electric heating alloy | ||||||||
| property | type | Cr20Ni80 | Cr30Ni70 | Cr15Ni60 | Cr20Ni35 | Cr20Ni30 | ||
| Main chemical composition% | Ni | Rest | Rest | 55~61 | 34~37 | 30~34 | ||
| Cr | 20~23 | 28~31 | 15~18 | 18~21 | 18~21 | |||
| Fe | Rest | Rest | Rest | |||||
| Max continuous Temp.of element(℃) | 1200 | 1200 | 1150 | 1100 | 1100 | |||
| resistivity(mm²/m) | 1.09 | 1.09 | 1.12 | 1 | 1.04 | |||
| Density((g/cm³)) | 8.4 | 8.4 | 8.2 | 7.9 | 7.9 | |||
| Thermal conductivity(KJ/M.h℃) | 60.3 | 60.3 | 45.2 | 43.8 | 43.8 | |||
| Coefficient of liner expansion(a*10-5/℃) | 18 | 18 | 17 | 19 | 19 | |||
| Melting point (℃) | 1400 | 1400 | 1390 | 1390 | 1390 | |||
| Elongation(%) | 720 | 720 | 720 | 720 | 720 | |||
| Micrographic structure | Austenitic | Austenitic | Austenitic | Austenitic | Austenitic | |||
| Magnetic property | NONE | NONE | NONE | NONE | NONE | |||
| Alloy Nomenclature/Performance | Cr20Ni80 | Cr30Ni70 | Cr15Ni60 | Cr20Ni35 | Cr20Ni30 | |
| Main Chemical composition | Ni | Rest | Rest | 55.0-61.0 | 34.0-37.0 | 30.0-34.0 |
| Cr | 20.0-23.0 | 28.0-31.0 | 15.0-18.0 | 18.0-21.0 | 18.0-21.0 | |
| Fe | ≤1.0 | ≤1.0 | Rest | Rest | Rest | |
| Max. continuous service temp. of element | 1200 | 1250 | 1150 | 1100 | 1100 | |
| Resistivity at 20°C(μΩ·m) | 1.09 | 1.18 | 1.12 | 1 | 1.04 | |
| Density (g/cm3) | 8.4 | 8.1 | 8.2 | 7.9 | 7.9 | |
| Thermal conductivity(KJ/m·h·°C) | 60.3 | 45.2 | 45.2 | 43.8 | 43.8 | |
| Coefficient of lines expansion(α×10-6/°C) | 18 | 17 | 17 | 19 | 19 | |
| Melting point (approx.)( °C) | 1400 | 1380 | 1390 | 1390 | 1390 | |
| Elongation at rupture (%) | >20 | >20 | >20 | >20 | >20 | |
| Micrographic structure | austenite | austenite | austenite | austenite | austenite | |
| Magnetic properties | nonmagnetic | nonmagnetic | nonmagnetic | Weak magnetic | Weak magnetic | |
| Alloy Nomenclature/Performance | Cr20Ni80 | Cr30Ni70 | Cr15Ni60 | Cr20Ni35 | Cr20Ni30 | |
| Main Chemical composition | Ni | Rest | Rest | 55.0-61.0 | 34.0-37.0 | 30.0-34.0 |
| Cr | 20.0-23.0 | 28.0-31.0 | 15.0-18.0 | 18.0-21.0 | 18.0-21.0 | |
| Fe | ≤1.0 | ≤1.0 | Rest | Rest | Rest | |
| Max. continuous service temp. of element | 1200 | 1250 | 1150 | 1100 | 1100 | |
| Resistivity at 20°C(μΩ·m) | 1.09 | 1.18 | 1.12 | 1 | 1.04 | |
| Density (g/cm3) | 8.4 | 8.1 | 8.2 | 7.9 | 7.9 | |
| Thermal conductivity(KJ/m·h·°C) | 60.3 | 45.2 | 45.2 | 43.8 | 43.8 | |
| Coefficient of lines expansion(α×10-6/°C) | 18 | 17 | 17 | 19 | 19 | |
| Melting point (approx.)( °C) | 1400 | 1380 | 1390 | 1390 | 1390 | |
| Elongation at rupture (%) | >20 | >20 | >20 | >20 | >20 | |
| Micrographic structure | austenite | austenite | austenite | austenite | austenite | |
| Magnetic properties | nonmagnetic | nonmagnetic | nonmagnetic | Weak magnetic | Weak magnetic | |